MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 6066-T6; 6066-T651
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A96066; Aluminium 6066-T651; AA6066-T6; Al6066-T6
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.72 g/cc0.0983 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 120120AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 150150Converted from Brinell Hardness Value
Hardness, Rockwell A 4747Converted from Brinell Hardness Value
Hardness, Rockwell B 7575Converted from Brinell Hardness Value
Hardness, Vickers 137137Converted from Brinell Hardness Value
Tensile Strength, Ultimate 393 MPa57000 psiAA; Typical
Tensile Strength, Yield 359 MPa52000 psiAA; Typical
Elongation at Break 12 %
@Diameter 12.7 mm
12 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 110 MPa
@# of Cycles 5.00e+8
16000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 70 %70 %0-100 Scale of Aluminum Alloys
Shear Modulus 26.0 GPa3770 ksiEstimated from similar Al alloys.
Shear Strength 234 MPa34000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000465 ohm-cm
@Temperature 20.0 °C
0.00000465 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  23.2 µm/m-°C
@Temperature 20.0 - 100 °C
12.9 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 24.8 µm/m-°C
@Temperature 20.0 - 300 °C
13.8 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.887 J/g-°C0.212 BTU/lb-°F
Thermal Conductivity 147 W/m-K1020 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 562.8 - 646.1 °C1045 - 1195 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 562.8 °C1045 °FAA; Typical
Liquidus 646.1 °C1195 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 414 °C778 °Fhold at temperature 2 to 3 hr
Solution Temperature 532 °C990 °Ffollowed by quenching
Aging Temperature 177 °C350 °Fhold at temperature 8 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 93 - 97 %93 - 97 %As remainder
Chromium, Cr <= 0.40 %<= 0.40 %
Copper, Cu 0.70 - 1.2 %0.70 - 1.2 %
Iron, Fe <= 0.50 %<= 0.50 %
Magnesium, Mg 0.80 - 1.4 %0.80 - 1.4 %
Manganese, Mn 0.60 - 1.1 %0.60 - 1.1 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.90 - 1.8 %0.90 - 1.8 %
Titanium, Ti <= 0.20 %<= 0.20 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6063-T6
Aluminum 6066-T4; 6066-T451
6060 Aluminum Composition Spec
Aluminum 6082-T6

MA6066T6 / 9409

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.