MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Toyobo Fortron® FX515T1 PPS, Impact Modified, 15% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS) with 20% Glass Fiber Filler

Material Notes: Product Description: Forton FX515T1 is a 15% glass filled, impact modified PPS grade with good impact resistance suitable for injection molding and food contact applications.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Additive: Impact Modifier

Features: Impact Modified

Uses: Automotive Applications

Automotive Specifications: RENAULT UB02b

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.37 g/cc0.0495 lb/in³ISO 1183
Maximum Moisture Content 0.0500.050
Linear Mold Shrinkage, Flow 0.0060 cm/cm0.0060 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0030 cm/cm0.0030 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 100 MPa14500 psiISO 527-2/5
Elongation at Break 2.1 %2.1 %ISO 527-2/5
Tensile Modulus 6.00 GPa870 ksiISO 527-1
Flexural Strength 150 MPa21800 psiISO 178
Flexural Modulus 5.80 GPa841 ksiISO 178
Flexural Strain at Break 3.1 %3.1 %ISO 178
Charpy Impact Unnotched 3.99 J/cm²19.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.01 J/cm²4.80 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 220 °C428 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Feed Temperature 66.1 - 71.1 °C151 - 160 °FInjection
Rear Barrel Temperature 304 - 310 °C579 - 590 °F
Middle Barrel Temperature 313 - 316 °C595 - 601 °F
Front Barrel Temperature 313 - 316 °C595 - 601 °F
Nozzle Temperature 299 - 310 °C570 - 590 °F
Zone 4 299 - 310 °C570 - 590 °FInjection
Melt Temperature <= 320 °C<= 608 °F
Mold Temperature 116 - 121 °C241 - 250 °F
Drying Temperature 121 °C250 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour
Back Pressure <= 3.50 MPa<= 508 psi
Screw Speed 45 rpm
@Thickness 40.6 mm
45 rpm
@Thickness 1.60 in

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHCQ6285 / 310978

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.