MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Titanium Grade 2
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Information provided by Allvac and the references.

Characteristics: Higher ductility, lower strength when compared to Ti alloys

Applications: Airframe components, cryogenic vessels, heat exchangers, CPI equipment, condenser tubing, pickling baskets.

Forms typically available: billet, bar, plate, sheet, strip, rod, wire, extrusions, tubing.

Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.

Key Words: ASTM Grade 2; UNS R50400, CP titanium, C.P. titanium alloy
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.51 g/cc0.163 lb/in³
 
Chemical PropertiesMetricEnglishComments
Thermal Neutron Cross Section 5.6 barns/atom5.6 barns/atomAverage for naturally occurring Ti
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 200200
Hardness, Knoop 170170
Hardness, Rockwell B 8080
Hardness, Vickers 145145
Tensile Strength  103 - 138 MPa
@Temperature 540 °C
14900 - 20000 psi
@Temperature 1000 °F
 131 - 186 MPa
@Temperature 425 °C
19000 - 27000 psi
@Temperature 797 °F
 172 - 207 MPa
@Temperature 315 °C
24900 - 30000 psi
@Temperature 599 °F
 207 - 228 MPa
@Temperature 205 °C
30000 - 33100 psi
@Temperature 401 °F
Tensile Strength, Ultimate 344 MPa49900 psi
Tensile Strength, Yield 276 - 448 MPa40000 - 65000 psi
 62.0 - 76.0 MPa
@Temperature 540 °C
8990 - 11000 psi
@Temperature 1000 °F
0.2% offset
 76.0 - 103 MPa
@Temperature 425 °C
11000 - 14900 psi
@Temperature 797 °F
0.2% offset
 90.0 - 124 MPa
@Temperature 315 °C
13100 - 18000 psi
@Temperature 599 °F
0.2% offset
 138 - 152 MPa
@Temperature 205 °C
20000 - 22000 psi
@Temperature 401 °F
0.2% offset
Elongation at Break 20 %20 %
 24 - 28 %
@Temperature 425 °C
24 - 28 %
@Temperature 797 °F
In 50 mm
 30 - 35 %
@Temperature 540 °C
30 - 35 %
@Temperature 1000 °F
In 50 mm
 30 - 38 %
@Temperature 315 °C
30 - 38 %
@Temperature 599 °F
In 50 mm
 38 - 45 %
@Temperature 205 °C
38 - 45 %
@Temperature 401 °F
In 50 mm
Reduction of Area 30 %30 %
 55 - 65 %
@Temperature 205 °C
55 - 65 %
@Temperature 401 °F
 70 - 80 %
@Temperature 315 °C
70 - 80 %
@Temperature 599 °F
 70 - 80 %
@Temperature 425 °C
70 - 80 %
@Temperature 797 °F
 70 - 80 %
@Temperature 540 °C
70 - 80 %
@Temperature 1000 °F
Tensile Modulus 103 GPa14900 ksi
Compressive Modulus 110 GPa16000 ksi
Poissons Ratio 0.370.37
Fatigue Strength  300 MPa
@# of Cycles 1.00e+7
43500 psi
@# of Cycles 1.00e+7
unnotched
 425 MPa
@# of Cycles 30000
61600 psi
@# of Cycles 30000
Unnotched
Fracture Toughness 66.0 MPa-m½60.1 ksi-in½K(Q); annealed
Shear Modulus 45.0 GPa6530 ksi
Izod Impact 114 - 171 J84.1 - 126 ft-lb
Charpy Impact  100 J
@Temperature 200 °C
73.8 ft-lb
@Temperature 392 °F
Notched
 115 J
@Temperature 300 °C
84.8 ft-lb
@Temperature 572 °F
Notched
 115 J
@Temperature 100 °C
84.8 ft-lb
@Temperature 212 °F
Notched
 160 J
@Temperature 0.000 °C
118 ft-lb
@Temperature 32.0 °F
Notched
 175 J
@Temperature -100 °C
129 ft-lb
@Temperature -148 °F
Notched
Coefficient of Friction, Dynamic 0.680.68Ti sliding on Ti; 300 m/min
 0.800.80Ti sliding on Ti; 40 m/min
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000520 ohm-cm0.0000520 ohm-cm
Magnetic Permeability 1.000051.00005at 1.6 kA/m
Magnetic Susceptibility 4.0e-84.0e-8kg; Paramagnetic
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 325 J/g140 BTU/lbHigh Purity Ti.
CTE, linear  8.60 µm/m-°C
@Temperature 0.000 - 100 °C
4.78 µin/in-°F
@Temperature 32.0 - 212 °F
 9.20 µm/m-°C
@Temperature 0.000 - 315 °C
5.11 µin/in-°F
@Temperature 32.0 - 599 °F
average
 9.70 µm/m-°C
@Temperature 0.000 - 540 °C
5.39 µin/in-°F
@Temperature 32.0 - 1000 °F
perpendicular to the c-axis
Specific Heat Capacity  0.523 J/g-°C
@Temperature 20.0 °C
0.125 BTU/lb-°F
@Temperature 68.0 °F
 0.560 J/g-°C
@Temperature 200 °C
0.134 BTU/lb-°F
@Temperature 392 °F
 0.620 J/g-°C
@Temperature 400 °C
0.148 BTU/lb-°F
@Temperature 752 °F
 0.670 J/g-°C
@Temperature 540 °C
0.160 BTU/lb-°F
@Temperature 1000 °F
 0.690 J/g-°C
@Temperature 600 °C
0.165 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity 16.4 W/m-K114 BTU-in/hr-ft²-°Fannealed
Melting Point <= 1665 °C<= 3029 °F
Liquidus 1665 °C3029 °F
Beta Transus 913 °C1680 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.30
@Temperature 710 °C
0.30
@Temperature 1310 °F
High purity Ti
Reflection Coefficient, Visible (0-1) 0.560.56High purity Ti; visible light.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.30 %<= 0.30 %
Nitrogen, N <= 0.030 %<= 0.030 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.25 %<= 0.25 %
Titanium, Ti >= 98.885 %>= 98.885 %
 
Descriptive Properties
Crystal Structurebccabove 913°C
 cphbelow 890°C

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 2, Annealed
Titanium Grade 1
Titanium Grade 4
Titanium Ti-6Al-4V (Grade 5), Annealed
Aluminum 6061-T6; 6061-T651

MTU020 / 14259

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.